CB4
Standard: CC495K
International Standards: more info
Composition in % (Mass fraction)
| % min. | % máx | |
|---|---|---|
| Cua | 78 | 82 |
| Ni | 2 | |
| P | 0,1 | |
| Pb | 8 | 11 |
| Sn | 9 | 11 |
| Zn | 2 | |
| Al | 0,01 | |
| Fe | 0,25 | |
| Mn | 0,2 | |
| S | 0,1 | |
| Sb | 0,5 | |
| Si | 0,01 |
a Including nickel
CB4
Standard: CC495K
| Casting process and designation | GC | GZ |
|---|---|---|
| Tensile Strength Rm N/mm2 min. |
220 | 220 |
| Yield point 0,2% Rp0,2 N/mm2 min. | 110 | 110 |
| Elongation A % min. | 8 | 6 |
| Brinell hardness HBW min. | 70 | 70 |
CB4
Standard: CC495K
| Density kg/dm3 | 9 |
|---|---|
| Specific heat j/g. k | 0,376 |
| Terminal expansion 10-6 k | 18,7 |
| Thermal conductivity W/m. ºk | 54 |
| Electrical conductivity m / (Ohm.mm2) | 6 |